High filling copper acid process

Your current location: Home >> news >> Industry news

High filling copper acid process

Data:2017-06-08 00:00 Source:http://en.hdrrunda.com Click:

High filling copper acid process

A, features,

 

1, the introduction of foreign advanced technology and raw materials, light speed is fast, go in a good position, with an excellent low electric leveling ability. 

2, the bath is stable, easy to control, easy to operate, light agent consumption is small. 

 

3, the operating temperature range is wide, 20-40℃ can obtain better results. 

 

4, coating light consistent, not easy to produce pinhole. 

  

Second, the plating process of high filling acid copper process

 

Dividing range standard

 

Copper CuSO4∙5H2O (g/L) 180-220 200

 

Sulfuric acid H2SO4 (g/L) 50-80 70

 

The chloride ion, CL- (mg/L) 60-150, 100

 

Hdr-68a (ml/L) 0.4-0.6 0.6

 

Hdr-68b (ml/L) 0.3-0.5 0.5

 

Hdr-68mu (ml/L) 6-10 8

 

Temperature (℃) 20-40 28

 

Anode current density (A/dm2) 1-6

 

Cathode current density (A/dm2) 1.5-8

 

Air stirring

 

Voltage (V) 3 minus 9

 

Preparation method of plating solution

 

1. Inject two-thirds of the pure water into the reserve tank (check whether the pure water contains chlorine ions). 

 

2. Add the amount of copper sulfate required by the opening cylinder and stir to dissolve. 

 

3. Add the required analysis pure sulfuric acid. 

 

4. Add high-purity activated carbon powder (2-5g/L), stir for 4 hours, set aside and filter. 

 

5, electrolysis for 6 hours, adding the amount of chlorine ions and additives needed to open the cylinder. 

 

6. Normal production can be achieved after qualified plating. 

 

Iv. Consumption: high filling copper acid process is calculated as per thousand ampere-hour consumption

 

Hdr-68a: 50 ~ 70ml / 1000 ampere-hour

 

Hdr-68b: 30 ~ 50ml / 1000 ampere-hour

 

Hdr-68mu: 60 ~ 80ml / 1000 ampere-hour

 

Ss ="font1">T impurity removal water: suitable for nickel plating agent, especially for zinc-based alloy parts, can remove heavy metal impurities in nickel plating solution.

In particular, direct addition of zinc has a significant effect.

Usage: 0.3 ~ 0.6 ml/l

3, hdr-28p high speed leveling agent: when the plating requirements are particularly good leveling, with the main light agent at the same time, you can get a particularly bright and plump coating.Generally press the main light agent consumption of 10%.

Five, points for attention

Welcome to contact our company (0755-28489710) before opening the new cylinder or using our company's brightening agent to turn the cylinder, and take the plating solution to our company's laboratory for analysis.